All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 10.00
Lithium Carbonate 10.00
Nepheline Syenite 62.00
Grolleg Kaolin 18.00
Add Amount
Copper Carbonate 2.00
Rutile 5.00

Instructions

Published in "Cone 6-10 Glazes" in the Jan 2015 issue of Ceramics Monthly.

A matte glaze with a variegated color surface.
After mixing the dry ingredients and adding water, screen with at least an 80-mesh sieve to remove lumps and disperse any colorants evenly.