All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax 5.00
Minspar 200 Feldspar 10.00
Nepheline Syenite 25.00
Georgia Kaolin 20.00
OM 4 Ball Clay 20.00
Silica 20.00
Add Amount
Zircopax 5.00

Instructions

This recipe was published in the June/July/August 2018 issue of Ceramics Monthly.


Mix borax separately with hot water and add to the wet glaze mix, then sieve. I mix this slip to a heavy cream consistency. For use on bisque ware. I bisque fire to cone 08. Glaze can be applied over the slip.