All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 26.32
EPK Kaolin 26.32
OM 4 Ball Clay 47.36
Add Amount
Bentonite 5.26

Instructions

Originally published in the May 2018 issue of Ceramics Monthly.
Mix the slip to a thicker consistency, then add water to your preference. For slip trailing application, fill slip trailing bottle with thick slip and add water as needed.