All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Spodumene 3.30
Talc 9.91
Whiting 11.79
Gerstley Borate 15.09
Custer Feldspar 22.64
Ferro Frit 3124 4.72
Kaolin 13.21
Silica 19.34
Add Amount
Bentonite 1.89
Zircopax 7.55
Mason Stain 6450 Praseodymium 3.00

Instructions

Published in "In the Potter's Kitchen: Easy and Elegant Butter Dish," in the July/August 2018 issue of Pottery Making Illustrated.

The image shown here has multiple glazes on it.

This recipe can be poured or brushed on with great results.