All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 5.85
Gerstley Borate 13.37
Whiting 8.10
Zinc Oxide 3.90
Custer Feldspar 44.39
EPK Kaolin 4.88
Silica 19.51
Add Amount
Zircopax 10.00

Instructions

Nice stable glaze that doesn't shift or run at cone 5.

Published in "Studio Takada" by Kaname and Sumiko Takada, in the March 2017 issue of Ceramics Monthly.