All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 6.00
Ferro Frit 3110 77.00
EPK Kaolin 7.00
Silica 10.00
Add Amount
Copper Carbonate 2.00
Bentonite 3.00

Instructions

Originally published in the May 2018 issue of Ceramics Monthly.