All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barnard Clay 24.00
EPK Kaolin 24.00
Hawthorne Clay 24.00
Newman Red Clay 24.00
Alumina Hydrate 4.00
Add Amount
Coarse Sand 5.00
Sawdust 5.00

Instructions


Mix to a clay-like consistency and use to separate pots from shelf. May also be molded into disks or other shapes and placed in between pots.

This recipe was shared by Stuart Gair in the April 2021 issue of Ceramics Monthly.