All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 2.80
Whiting 32.50
Ferro Frit 3124 14.90
Alberta Slip 19.10
EPK Kaolin 24.70
Silica 6.00
Add Amount
Copper Carbonate 2.50
Bentonite 2.00

Instructions


This should be a thin to medium application.

This recipe was shared by Paul Briggs in the February 2021 issue of Ceramics Monthly.