Val Cushing Soft Satin Glossy Forrest Gard

You have read of of your complimentary recipes for the month.
For unlimited access to Ceramics Recipes premium content, please subscribe.
Yes, I want to subscribe to Ceramics RecipesAlready a digital subscriber? Log in now.
We understand your email address is private. You will receive emails and newsletters from Ceramic Arts Network. We will never share your information except as outlined in our privacy policy. You can unsubscribe at any time.

Please enjoy this complimentary recipe for the month.
For unlimited access to Ceramics Recipes premium content, please subscribe.
Yes, I want to subscribe to Ceramics RecipesNot right now. Continue to recipe. Already a digital subscriber? Log in now.
We understand your email address is private. You will receive emails and newsletters from Ceramic Arts Network. We will never share your information except as outlined in our privacy policy. You can unsubscribe at any time.

Subscribe
Ingredients
Instructions
Published in "In the Service of Food" by Adrienne Eliades, in the January/February 2017 issue of Pottery Making Illustrated.
Good base that holds colorants well. Try adding 2–10% colored stain for various colors.
I use a down-fire schedule for glaze firing to promote crystal growth. The Val Cusing Soft Satin Glossy glaze will go shiny when cooled too quickly.
Cone 6 glaze firing schedule: Ramp 1 (50F per hour to 180F), Ramp 2 (350F per hour to 2000F), Ramp 3 (150F per hour to 2210F, 10 minute hold), Ramp 4 (500F per hour to 1910F, 10 minute hold), and Ramp 5 (90F per hour to 1400F, 10 minute hold).
Recipe Topics
Clay Bodies and Casting Slips
Low Fire (Cone 022 – 01)
Mid Range (Cone 1 – 7)
High Fire (Cone 8 – 14)
Raku
Salt, Soda, and Wood
Slip, Engobe, and Terra Sigillata
Reference
Create your own Recipes!
You can keep your recipes private or share with others.
Create a Recipe
Manage your Recipes