All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 11.00
Lithium Carbonate 9.00
Whiting 9.00
Nepheline Syenite 44.00
EPK Kaolin 11.00
Silica 16.00
Add Amount
Titanium Dioxide 6.00
Bentonite 2.00

Instructions


This glaze will give a cream-colored matte surface when applied thinly and break into rivulets of gloss blue-white where thicker. Use with caution: it runs!

This recipe was shared by Marc Egan in the March/April 2020 issue of Pottery Making Illustrated.