All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 5.00
Ferro Frit 3124 6.00
Minspar 200 Feldspar 36.00
OM 4 Ball Clay 18.00
6 Tile Kaolin 20.00
Alumina Hydrate 5.00
Silica 10.00
Add Amount
Molochite 10.00

Instructions


This is a very durable and highly vitrified off white tile body. The molochite helps to mitigate warping, but is not 100% necessary.

This recipe was shared by Forrest Lesch-Middelton in the October 2020 issue of Ceramics Monthly.