All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 2.04
Gerstley Borate 3.06
Wollastonite 9.18
Whiting 14.30
Custer Feldspar 19.39
Barnard Clay 10.20
Cedar Heights Redart 29.59
EPK Kaolin 2.04
Silica 10.20
Add Amount
Red Iron Oxide 2.04

Instructions

Published in "Engobes to Celadons" the September 2016 issue of Ceramics Monthly.

This recipe was originally sourced form Cushing's Handbook by Val Cushing.