All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 6.31
Whiting 10.17
Zinc 5.90
Potash Feldspar 48.12
Silica 29.50
Add Amount
Bentonite 1.73

Instructions

Published in "Cone 10 Transparent" by Antoinette Badenhorst, in the June 2015 issue of Ceramics Monthly.

A transparent base glaze that can be used as a clear or with colorants. Fire to cone 10 for a stain finish. Try testing up to 10% commercial stains for different colors.
Mix all ingredients together prior to adding the water. Adding a small amount of valium chloride helps keep the glaze in suspension.