All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 23.50
Ferro Frit 3124 17.40
EPK Kaolin 18.30
Calcined Kaolin 13.90
Silica 26.90
Add Amount
Zircopax 5.00

Instructions


This recipe was shared by Dan Ingersoll in the May/June 2020 issue of Pottery Making Illustrated.