All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 5.00
Dolomite 6.00
Gerstley Borate 18.60
Red Iron Oxide 13.00
Talc 10.10
F-4 Feldspar (sub. Minspar 200) 32.70
EPK Kaolin 3.40
Silica 11.20
Add Amount
Crocus Martis 2.25

Instructions


This recipe was shared by Ryan Coppage in the November 2019 issue of Ceramics Monthly.