All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 9.26
Whiting (Pfizer Vicron 41-8) 15.74
Custer Feldspar 39.81
OM 4 Ball Clay 10.19
Silica 25.00
Add Amount
Cobalt Carbonate 3.24
Iron Oxide 2.78

Instructions

Published in "Cone 9 Glazes," in the March 2016 issue of Ceramics Monthly.

The piece in the image shown here has multiple glazes on it, including Tom Turner's Blue Teadust, Flambe, and a wash of iron oxide and water.
This glaze layers well with Tom Turner's Flambe glaze and iron-oxide wash.