All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Bone Ash 2.04
Talc 7.14
Whiting 19.39
Custer Feldspar 32.65
EPK Kaolin 9.19
Silica 29.59
Add Amount
Titanium Dioxide 3.06

Instructions

This recipe was shared in the January 2019 issue of Ceramics Monthly by Adrian King.
Apply to a medium thickness. This glaze will run when hot as well as when layered with other glazes. I soda fire this glaze to cone 10–11 reduction in a gas-fired kiln.