All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 40.47
Barium Carbonate 30.95
Whiting 9.53
OM 4 Ball Clay 7.14
Titanium Dioxide 7.14
Tin Oxide 4.76

Instructions

This glaze is from Diane Creber's book, "Crystalline Glazes".

The test tile is B-Mix fired in oxidation.  (In reduction, the glaze is a cream color with a nice satin surface.)
Probably should be considered not food-safe.