All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 7.80
Custer Feldspar 51.10
EPK Kaolin 12.20
Silica 28.90
Add Amount
Red Iron Oxide 10.00
Bentonite 1.00

Instructions

Published in "Throw Some Clay on the Walls" by Gary Jackson, in the March/April 2016 issue of Pottery Making Illustrated, page 26.

The Tenmoku glaze shown on the piece in the image here was fired to cone 10 in a reduction/soda kiln.