All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 19.70
Whiting 2.60
Custer Feldspar 35.00
EPK Kaolin 22.70
Silica 20.00
Add Amount
MS Best Black 6600 6.00

Instructions


I use Mason Stain (MS) Best Black, but other colorants may work with testing. Applied thin it resembles gun metal, applied thick it's a semi-matte charcoal. Stir frequently or add bentonite.