All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.00
Custer Feldspar 35.00
Kentucky Ball Clay (OM 4) 15.00
Silica 30.00

Instructions

Published in "My Way With Clay" by Rick Malmgren, in the Oct 2000 issue of Ceramics Monthly.
A cone 10 that works equally well at cone 6; yields yellow "tea dust" crystals in reduction.  Not as interesting in oxidation; just lies there and looks brown.