All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 1.00
Ferro Frit 3110 15.80
Cobalt Carbonate 2.10
Copper Carbonate 38.40
Red Copper Oxide 38.40
Red Iron Oxide 4.30

Instructions

Published in "Resist Erosion Raku" in the September/October 2016 issue of Pottery Making Illustrated.
Red copper oxide has a coating on it to avoid oxidation, and will cause a film to appear on top of the hydrated solution. After hydrating, add a few drops of Dawn dish soap to disperse this film.