All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 24.00
Nepheline Syenite 47.00
EPK Kaolin 5.00
Silica 24.00

Instructions


The variation in the glaze is achieved through the reduction firing. All colors in the imagery are underglazes. The advantage of both the slip and glaze I use is their firing range. The glaze melts at cone 4 and tolerates cone 9, which is great for a small updraft gas kiln.

This recipe was shared by Jennifer Graff in the September 2021 issue of Ceramics Monthly.