All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Ferro Frit 3124 76.59
EPK Kaolin 12.77
Silica 10.64
Add Amount
Zircopax 10.64

Instructions

Published in "Cone 6-10 Glazes" in the Jan 2015 issue of Ceramics Monthly.

This is a stiff white glaze.
Apply thick, fire on medium speed to cone 04, hold for 5 minutes at top temperature.