All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Soda Ash 3.12
Custer Feldspar 13.79
Nepheline Syenite 47.23
Spodumene 11.81
EPK Kaolin 2.74
OM 4 Ball Clay 15.68
Cedar Heights Redart 5.63

Instructions


Adjust the amount of Redart for color variations. Dissolve the soda ash in 1 quart of water, then add it to the glaze. Apply thin for a metallic gold and orange with crystals. Apply thick for a creamy white that blushes orange and showcases wood-ash deposits.

This recipe was shared by Trevor Youngberg in the April 2020 issue of Ceramics Monthly.