All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 4.00
Gerstley Borate 6.00
Lithium Carbonate 1.00
Soda Ash 4.00
Whiting 13.00
Custer Feldspar 51.00
Flint 21.00
Add Amount
Bentonite 2.00
Titanium Dioxide 4.00
Copper Carbonate 5.00

Instructions

This glaze was originally called "V.C. Karren Starshine Aqua Copper" and was published in Ceramics Monthly, March 2000.

The test tile is B-Mix fired in reduction.
Can be runny if applied thickly.