All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gillespie Borate 9.43
Soda Ash 15.09
Ferro Frit 3110 63.21
EPK Kaolin 4.72
Silica 7.55
Add Amount
Chrome Oxide 0.24
Copper Carbonate 2.83
Spanish Red Iron Oxide 9.43
Bentonite 1.89

Instructions


This glaze is runny when fired. I apply thickly, like Elmer's glue consistency, high on the pot so it can drip. Firing to cone 04 is ideal. The color shifts to olive green when fired to cone 03.

This recipe was shared by Lisa Orr in the November 2019 issue of Ceramics Monthly.