All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Calcium Carbonate 5.26
Dolomite 21.05
Spodumene 18.95
Custer Feldspar 28.42
EPK Kaolin 26.32
Add Amount
Tin Oxide 4.74

Instructions


Once pots are decorated with Hannah’s Fake Ash glaze, I then dip them in this glaze, which I mix to the consistency of heavy cream. It must be fired hot, to cone 10–11 in moderate to heavy reduction starting at cone 012.

This recipe was shared by Terry Plasket in the June/July/August 2021 issue of Ceramics Monthly.