All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Borax (dissolved in hot water) 5.90
OM 4 Ball Clay 47.00
EPK Kaolin 47.10
Add Amount
Zircopax 10.00

Instructions

Published in "Throw Some Clay on the Walls" by Gary Jackson, in the March/April 2016 issue of Pottery Making Illustrated, page 26.

This slip creates a great color companion to the natural warmth and browns of the soda clay after firing. The Smooth Orange Flashing Slip can be seen on the edges of the piece shown here.