All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 19.00
Gerstley Borate 4.00
Wollastonite 5.50
Custer Feldspar 28.50
EPK Kaolin 28.00
Silica 15.00
Add Amount
Zircopax 10.00

Instructions


Add enough water to make the glaze slurry a thick cream consistency. Sieve with an 80-mesh screen prior to use.

This recipe was shared by Natasha Alphonse in the June/July/August 2021 issue of Ceramics Monthly.