All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Wollastonite 26.17
Ferro Frit 3124 34.97
EPK Kaolin 33.96
Silica 4.90

Instructions


This clear glaze is used on the interior of my functional pieces. It blends well with the polished porcelain and isn't distracting to my carved designs. Recipe originally from Digitalfire (https://digitalfire.com).

This recipe was shared by Joann Axford in the September/October 2019 issue of Pottery Making Illustrated.