All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 17.00
Custer Feldspar 35.00
Ball Clay 17.00
Calcium Carbonate 12.00
Silica 19.00
Add Amount
Copper Carbonate 1.25

Instructions


This recipe is not food safe.

This recipe was sourced from The Ceramic Spectrum: A Simplified Approach to Glaze and Color Development by Robin Hopper.