All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 10.00
Wollastonite 20.00
Minspar 200 Feldspar 50.00
EPK Kaolin 10.00
Silica 10.00
Add Amount
Mason Stain 6097 Dark Red 10.00
Red Iron Oxide 30.00

Instructions

Published in "Montana Glazes," in the Jan 2016 issue of Ceramics Monthly.

The piece in the image shown here has Sensei Red glaze over black stoneware.
Apply only three brush coats, or a three-second dip application, or spray two even coats. Note: I spray two coats, let the glaze dry, then wipe the piece with a damp sponge to expose some of the black clay texture underneath.