All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Talc 17.00
Whiting 10.00
Ferro Frit 3134 20.00
Nepheline Syenite 30.00
EOK Kaolin 13.00
Silica 10.00
Add Amount
Zircopax 10.00

Instructions


This is a cone-6 glaze that I fire cone 8 (using a witness cone) and hold for 10 minutes at the end of the firing. This glaze is fairly stable, but runs a little when fired hot. It breaks over texture beautifully. Add Epsom salts to the wet mix to keep the particles suspended. Apply to the thickness of a dime.

This recipe was shared by Jen Allen in the March 2020 issue of Ceramics Monthly.