All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 12.50
Whiting 10.41
Nepheline Syenite 56.26
Silica 20.83
Add Amount
Copper Carbonate 0.80
Tin Oxide 1.50
Titanium Dioxide 2.00

Instructions

Published in "Opaque Glazes" by John Britt, in the Oct 2014 issue of Ceramics Monthly.