All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 5.00
Nepheline Syenite 65.00
EPK Kaolin 20.00
Silica 10.00

Instructions

Published in the May 2018 issue of Ceramics Monthly. This recipe is from Val Cushing’s Handbook. He states that this can also be used as a clay body with 1–2% bentonite added. The slip takes colorants well, and glaze can be applied on top of the slip.