All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 14.00
Calcium Borate Frit 16.00
Soda Feldspar 47.00
China Clay 5.00
Silica 18.00
Add Amount
Copper Oxide 2.00

Instructions

Published in "Cool Colors" by Linda Bloomfield, in the Feb 2012 issue of Ceramics Monthly.

 

Calcium borate frit is an English frit similar in composition to colemanite with some added silica. American frits such as Ferro 3124, 3134, or 3195 can be substituted but they contain less boron and more silica. 'Borax frit' contains sodium, calcium, and boron similar to Gerstley borate and can be substituted with Ferro 3124 or 3134.