All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 24.05
Gerstely Borate 4.01
Custer Feldspar 21.00
Spodumene 30.04
EPK Kaolin 8.93
Silica 11.97
Add Amount
Zircopax 5.04

Instructions


This is a matte dipping glaze, which should measure 55 SPG on a hydrometer, or visually look like half-and-half cream. Thoroughly mix before using, as the spodumene will settle in the bottom of the bucket. I fire in gas reduction, and turn off the kiln when cone 7 bends to 2 o’clock. In oxidation, the appearance will be more translucent and less white.

This recipe was shared Dodie Campbell in the May/June 2021 issue of Pottery Making Illustrated.