All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Barium Carbonate 7.10
Whiting 14.30
Zinc Oxide 7.10
Kona F-4 Feldspar 35.70
Nepheline Syenite 21.40
EPK Kaolin 14.40
Add Amount
copper Carbonate 0.50

Instructions

Published in "Cone 10 Glazes" by Holly Hanessian, in the Feb 2017 issue of Ceramics Monthly.
Substitute Minspar 200 Feldspar for the Kona F-4 Feldspar. This glaze works best when applied quite thinly. When surrounded by tiles glazed with John Britt's Nickel Yellow glaze during the firing, the Sam Chung's Satin Mint changed slightly in color.