All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Dolomite 15.10
Whiting 11.30
G-200 Feldspar 30.70
EPK Kaolin 16.00
Silica 26.90
Add Amount
Bentonite 2.00
Yellow Iron Oxide 2.00
Zircopax 1.00

Instructions

Published in "The Strong Silent Type: Michael McCarthy's Quiet Craftmanship" by Scott Norris, in the Feb 2008 issue of Ceramics Monthly.