All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 6.90
#6 Tile Kaolin 48.28
Grolleg Kaolin 10.34
Silica 34.48
Add Amount
Bentonite 1.00

Instructions

Published in "Recipes for Salt & Soda" in the Feb 2015 issue of Ceramics Monthly.

A reddish tan slip or engobe made for application to bisque fired ware.
Made for application to bisque fired ware. Test first if applying to leather hard clay or greenware.