All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Lithium Carbonate 0.54
Strontium Carbonate 21.67
Nepheline Syenite 63.30
EPK Kaolin 6.66
Silica 7.83
Add Amount
Copper Carbonate 1.00

Instructions

This recipe was shared by Joe Molinaro in "Cone 6–11 Recipes" in the November 2018 issue of Ceramics Monthly.
A nice copper blue with a smooth buttery matte surface. A wide variety of stains and colorants can be used effectively with this glaze.