All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Soda Feldspar 35.00
Magnesium Carbonate 25.00
Ferro Frit 3195 10.00
Talc 15.00
Kaolin 15.00
Add Amount
Chromium Oxide 5.00

Instructions

Published in "Reticulation Glazes" by Robin Hopper, in the May/Jun 2009 issue of Pottery Making Illustrated.


The tile above shows the recipe without the colorant added. Putting the reticulation glazes over a colored slip allows the top glaze to move and the visible cracks to be colored between "islands" of glaze. Any colored slip will do, but one of the most interesting is usually black, as it intensifies the color of the covering glaze.

With reticulation glazes applied heavily over the slip and fired at cones 04, 6 and 9-10, and with added colorants, a wide range of textural possibilities can be developed.