All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.00
Nepheline Syenite 18.00
Ferro Frit 3134 14.00
OM-4 Ball Clay 18.00
Silica 30.00
Add Amount
Tin Oxide 7.50
Chrome Oxide 0.20

Instructions

Published in "Four Ways to Red" by Dave Finkelnburg, in the Apr 2011 issue of Ceramics Monthly.