All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Nepheline Syenite 45.00
Soda Feldspar 10.00
OM-4 Ball Clay 15.00
EPK 10.00
Soda Ash 19.00
Add Amount
Redart 6.00
Rutile 10.00

Instructions

This is version of a popular shino recipe developed by Quinn Maher.

 