All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Custer Feldspar 23.00
Pryophyllite 8.00
6 Tile Clay 26.00
Ball Clay 8.00
EPK Kaolin 20.00
Silica 15.00
Add Amount
Bentonite 2.00
Epsom Salts 0.25

Instructions

Published in "Blending the Lines" by Kenyon Hansen, in the Jul/Aug 2014 issue of Pottery Making Illustrated.