All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
EPK Kaolin 25.00
G-200 Feldspar 25.00
OM 4 Ball Clay 25.00
Silica 25.00

Instructions


This slip can be applied in various consistencies. I add water and mix until it achieves a creamy, milkshake thickness. I apply two coats for an opaque background on my forms. This slip fits any clay body from low fire to high fire.

This recipe was shared by Sara Ballek in the November/December 2020 issue of Pottery Making Illustrated.