All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Gerstley Borate 8.30
Strontium Carbonate 12.10
Wollastonite 16.10
Nepheline Syenite 40.10
EPK Kaolin 11.40
Silica 12.00
Add Amount
Zircopax 3.50
MS 6001 Alpine Rose 2.10
MS 6404 Vanadium Yellow 1.00
MS 6129 Golden Ambrosia 1.70
MS 6117 Red Iron 0.40
MS 6031 Salmon 2.30

Instructions

Published in "Following a thread: Matte Glazes at Mid Range," in the November 2015 issue of Ceramics Monthly, page 61.
Mix to a specific gravity of 1.42.