All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
6 Tile Clay 66.67
Silica 33.33
Add Amount
Mason Stain 6026 6.67
Bentonite 5.56

Instructions


The slip base used for the pink also works with other stains, so allow yourself to experiment. Its application can be rather thick, about the consistency of heavy cream. Use any transparent glaze to finish.

This recipe was shared by Jason Hartsoe in the September/October 2021 issue of Pottery Making Illustrated.