All recipes are displayed as ratios, unless "in parts" is included in the recipe. You can adjust the recipe for larger or smaller batches by adjusting the total below the recipe. For example, for a 10,000-gram batch, put “10,000” in the box. Have more questions? View our help page here or watch a video tutorial here. 

Ingredients

Ingredient Amount
Whiting 20.00
Ferro Frit 3134 14.00
Nepheline syenite 18.00
OM4 Ball Clay 18.00
Silica 30.00
Add Amount
Tin Oxide 7.50

Instructions

Published in "Cone 6-10 Glazes" in the Jan 2015 issue of Ceramics Monthly.

Shiny at all temperatures, gets darker pink as the glaze gets thicker, white where very thin. I fire this to cone 9, at cone 8 it is a darker pink. At cone 10 it is almost white.
Mix all dry ingredients together prior to adding the water. Do not omit the tin oxide from this recipe. It is responsible for making the glaze pink as well as opaque. Do not substitute another opacifier (like zircopax/zirconium silicate), only tin oxide will work.